You may have to evaluate the heat treated conditions and mechanical properties for each and combination of two metals before the welding. Here is the brief summary.
1. Weldability of SCM 440 (AISI 4140) ; Similar Welds
If the SCM 440 was hardened & tempered or flame (or nitrided/induction) hardened, the fusion welding may be very difficult or impossible. If they are not hardened material, the welding is possible when you use ER 80S-B2 or E8016-B2 with preheat (min. 200C) and interpass temperature (max. 316C) followed by PWHT.
2. Weldability of SA352 LC2-1 ; Similar Welds
It may show a good weldability when you use the appropriate welding electrodes (i.e., ER 80S-C2, E8016-C2, etc.) with preheat (min. 150C) and interpass temperature (max. 232C) followed by PWHT (when THK > 2inch).
3. Combination between SCM 440 (AISI 4140) and SA352 LC2-1 ; Dissimilar Welds
It may be impossible. It was one of the critical issues of API RP 582 committee, but there is no solution yet.
As a result, the welding in this combination should be avoided unless you have a certified WPS/PQR.
몇 년 전에 한 번 만나 뵈었던 것 같습니다. Spheric Tank 적용 용접 재료(XL-550) 승인 문제로...(S-Tank 사와 함께) 잘 지내셨는지요?
두 박사님들 조언에 끼어 들 형편은 아니지만, 저는 현장을 충분히 고려한다면 Inconel 82 을 추천드립니다. 관리적인 측면은 정확한 WPS를 얘기하지만, 막상 Maintenance 와 Shut Down 수리 공사에서 정확한 WPS를 현장에 100% 반영할 수 있는 부분은 좀 어렵지 않나 싶습니다. 강도적인 측면이 걱정된다면 SUS 312(H)-Modified 계열로 내크랙성도 확보하고 강도도 확보하고(120,000ksi TS)...
Shaft Key Hole 자리(외경 링 열박음 장치)는 자주 파손되어 샤프트와 링이 헛돌아 큰 사고를 내기도 하는데(시멘트 Plant에는 2000 dia 이상 되는 부품들이 많습니다), 긴급 Maintenance는 일단 용접을 완벽하게 끝내는 게 가장 Key 이지 않겠습니까? 그리고, 이 부분이 장기적으로 걱정된다면 Spare 를 얼른 기안하셔서 확보하시는 것도...
I believe the crack may be mostly taken place during welding. Even though the crack is not occured during welding, some post-cracks are expected during operation (due to the stress concentrated at the weld joint).
1. 두재질 용접시 강도가 문제가 되서 문제가 발생되는지요
2. 두재질 용접후 열처리로 인해 문제가 발생되는지요
3. inconel 625(ERNICRMO-3) 또는 INCONEL80(ERNICR-3)
용접봉을 사용하면 어떨런지요
4. 한쪽을 BUTTERING 용접후 용접을 하면 어떨런지요
Q1. 두재질 용접시 강도가 문제가 되서 문제가 발생되는지요.
A1 [Thomas Eun] Not directly related with the weldability. But the strength and hardness are generally very important factors for shaft material.
Q2. 두재질 용접후 열처리로 인해 문제가 발생되는지요.
A2. [Thomas Eun] It is not a big issue. But the welding itself may be very difficult or impossible due to the crack.
Q3. inconel 625(ERNICRMO-3) 또는 INCONEL80(ERNICR-3) 용접봉을 사용하면 어떨런지요.
Q4. 한쪽을 BUTTERING 용접후 용접을 하면 어떨런지요.
A3/A4. [Thomas Eun] It may not have sufficient benefit due to strength, hardness, density and somewhat weldability.
I believe the best way at this state will be the friction-welding if it is available.
Alternative welding as an unproved method (as a pilot test welding) : If the SCM440 is not hardened material, the temper (or half) bead welding between SCM440 and SA352 LC2-1 may be recommended with ER 80S-B2 or E8016-B2, preheat (min. 200C) and interpass temperature (max. 316C) followed by PWHT. But the quality/result is not guaranteed.
용접봉 선정은 단순하게 두 재질의 차이만 가지고 평하기에는 너무 많은 선택이 발생할 수 있습니다.
그래서 용도를 명확하게 알아야 제대로 된 답변을 얻을 수 있지요.
3%Ni강이 맞다면 아마도 LPG나 LNG등의 저온용 강재일 것이고,
상대부재가 L.A이라면 적절한 강도가 함께 요구되는 것으로 판단합니다.
선택은 크게 두가지 입니다.
80혹은 90 계열의 고강도 용접재료를 쓸 것인지
아니면 Inconel이나 Hastelloy와 같은 저온 인성을 찾을 것인지..
둘중에 어느 것을 선정할 것인지는 설계 기준 (용도)에 따라 달라지겠지요.