profile 유정길 2005-08-05 19:24:58
2 478
nace mr0175 재질의 배관재 용접시 사용하여야 할 용접봉 사양을 알고 싶습니다.

이진희 2005-08-05 20:40

NACE Code에서 용접봉 선정과 관련된 특별한 규정은 사실상 없습니다.
Code상에는 Ni Content의 제한등이 언급되어 있지만, 예를 들어 A516-60을 용접한다고 하면, 그냥 E7016으로 용접하면 됩니다.
그냥 저수소계 용접봉을 구매하여 사용하시면 됩니다.
단, 용접부 경도 규정은 준수해야겠지요.

Thomas Eun 2005-08-21 04:13

You may have to consider the followings;

1. Is it correct the applicable standard, NACE MR0175?
Because more than 98% of needs in Korean industries including oversea projects are related in oil refinery plants, not oil & gas production.

2. What is your material?
Because the requirement is different per materials.

3. What is your concern in sour service? e.g., SSC or HIC (Blistering/Stepwise Cracking) or SOHIC

4. If you are concerning about oil refinery plants, the followings (Welding Point of View-Not base metal) are recommended.
4.1 To apply NACE MR0103-2003 (Only for SSC prevention of Several Materials)
(1) Hardness for base metal and weldments
(2) Carbon equivalent (Ceq) < 0.43%
(3) Ni content for base metal and weld metal : No restriction
4.2. To apply NACE publ.8X-194-1994 (For prevention of SSC or HIC or SOHIC of carbon steel only)
(1) All requirements in para.4.1
(2) Carbon equivalent (Ceq) <0.38% when V + Cb > 0.03% or each > 0.02%
(3) Strong NDE requirements -e.g., WFMT, UT on weldments

Please find the attachment for more detail information.

NACE Corrosion and Materials Selection/Design Specialist
thomaseun@hanmail.net (for Korean)


HydrogenDamage.pdf

(주)테크노넷|대표. 이진희|사업자등록번호. 757-88-00915|이메일. technonet@naver.com|개인정보관리책임자. 이진희

대표전화. 070-4709-3241|통신판매업. 2021-서울금천-2367|주소. 서울시 금천구 벚꽃로 254 월드메르디앙 1차 401호

Copyright ⓒ Technonet All rights Reserved.